1.7147 | 20MnCr5 |
20MnCr5 is low-carbon, chromium, carburizing steel with low case hardenability and low-to-medium core hardenability. This steel is available as hot worked and cold finished bar, rod, and wire; seamless mechanical tubing; and
Composition:
C | Si | Mn | p | s | Cr | Mo | Ni | B |
0,17-0,22 | 0,40 | 1,10-1,40 | 0,035 | 0,035 | 1,00-1,30 | – | – | – |
Hot working:
Forging temperature range: 1245-850℃
Note: Heat to 1245 ℃. Do not forge below 850.
Heat treatment:
Soft annealing | Heat treatment to obtain a certain structure | Heat treatment to obtain a certain tensile strength | Carburize | Core hardening | intermediate annealing | Surface hardening | Temper |
650-700 | 850-950 | 900-1000 | 900-950 | 850-880 | 810-840 | 170-210 |
Main application:
Average size cog wheels, arbors etc. for vehicle and gear building
Shape of product:
Round, flat, step shape, ring, disc, shaft, other shape depend on customer needs